Results 16 to 30 of 37
Thread: Backyard Phosphating
-
13th Jul 2019, 08:15 PM #16.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
Shades of Grey!!
Nearly two years ago I made an arbor ejector for the tool and cutter grinder's workhead inspired by the work of John " Shed". I thought I had used 1214 for both main components. My experiments this afternoon suggest maybe otherwise or that there are variations in the composition of 1214.
I was disappointed to find rust on both components when they had been stored in a lidded plastic container inside a cupboard so I thought that if phosphating does provide some corrosion resistance, there parts would be worthy recipients.
The parts when made in 2017 -
DSC_8154 (Large).jpg
And out of the box today -
IMG_20190713_142527758.jpg
After Rust-Offing with a non treated piece of 1214 for comparison.
IMG_20190713_160305744.jpg IMG_20190713_160909914.jpg
The disc took probably half an hour of constant swabbing, to achieve the pictured result. The bolt, about half that time.
BT
-
13th Jul 2019, 08:19 PM #17Member: Blue and white apron brigade
- Join Date
- Feb 2006
- Location
- Perth
- Posts
- 7,189
-
13th Jul 2019, 08:35 PM #18.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
-
13th Jul 2019, 08:39 PM #19Most Valued Member
- Join Date
- Nov 2007
- Location
- melbourne australia
- Posts
- 3,228
-
13th Jul 2019, 08:41 PM #20.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
-
13th Jul 2019, 09:05 PM #21Philomath in training
- Join Date
- Oct 2011
- Location
- Norwood-ish, Adelaide
- Age
- 59
- Posts
- 6,561
EN25 from memory. Nice stuff to machine and gives a good finish straight off the tool.
Not quite Bob. Looking at my Kaiser originals, they have the spigot bit left bare. Other than that, they are close, especially with the coating.
P1020271 (Medium).JPG
I did some reading and apparently phosphating does not work well with high nickel/ chromium steels. Could the disc be stainless?
Michael
-
13th Jul 2019, 10:27 PM #22.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
[QUOTE=Michael G
I did some reading and apparently phosphating does not work well with high nickel/ chromium steels. Could the disc be stainless?
Michael[/QUOTE]
Not stainless Michael.
Could be 1020 if it's not 1214 but if it is the former I would have thought the phosphoric would have taken effect quicker given the absence of lead.
Bob.
-
20th Jul 2019, 08:06 PM #23Member: Blue and white apron brigade
- Join Date
- Feb 2006
- Location
- Perth
- Posts
- 7,189
One week on
PAed pieces have been outside under back veranda and it has rained a fair bit in the last few days.
No sign of any rust on the second from the left piece (stripped back to bare steel and the in PA for 10 minutes)
Some small specs of rust on the pieces that were already partially rusted.
Oneweek.JPG
-
20th Jul 2019, 08:20 PM #24.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
The extra hundred metres or so you live from the Swan than me must make all the difference Bob !!!
I have rust forming on 1045, oiled and wrapped in a zip lock plastic bag and stored inside that metal drawer pedestal next to the mill. Strangely the test piece of phosphated and raw, lightly oiled, 1214 bar left exposed on the bench shows no signs of corrosion..... yet.
-
20th Jul 2019, 09:31 PM #25Golden Member
- Join Date
- Mar 2009
- Location
- Melbourne
- Age
- 54
- Posts
- 825
Not phosphating but this might be of interest.
Today I used some Birchwood Casey Super Blue I bought a few months ago for the first time and was pretty happy with the results.
Birchwood Casey Super Blue 01.jpg
The freshly machined part, plain old 1020 mild steel, after finishing it was sprayed with some brake cleaner to remove any oil then wiped dry with a towel .
Thiel X Feed Stop 1.jpg
The bluing compound was applied with an ear bud and a dark blue/black oxide layer appeared immediately on contact. The part was at ambient temperature which is not a lot here at the moment.
After fully coating the part it was left for about 30sec then rinsed under warm water. The result was as seen below.
Thiel X Feed Stop 2.jpg
Finally after rubbing on a coating of ISO68 oil, beginning to end took about five minutes.
Thiel X Feed Stop 3.jpg
I've got no idea how durable the coating is or of it's rust resisting properties but it's the quickest and easiest bluing I've ever done.
I usually flame blue parts like this and while the blue might not be as colourful it's nice and consistent.
The 90ml bottle was around $20.00 so not particularly cheap but you don't use a lot so there's enough there to last me a long while.
Cheers,
Greg.
-
20th Jul 2019, 10:28 PM #26.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
Hi Greg,
I've been using Super Blue for years for "cosmetic " touch ups. Extremely handy stuff. For blackening larger stuff I've tried my hand at acid fuming with the ever patient Bob L as my tutor.
IMG_20181124_153131059.jpg IMG_20181125_115655518.jpg
-
21st Jul 2019, 10:40 AM #27Member: Blue and white apron brigade
- Join Date
- Feb 2006
- Location
- Perth
- Posts
- 7,189
I'm starting to think your shed's brick walls might the culprit and might be giving off something that adds to the moisture and creates a more corrosive environment inside your shed.
One possibility I have in mind is what happened to the copper pipes attached to the HWS at mum and dad's unit in the mid 1990's. Not long after they moved in, the copper pipes immediately underground from the HWS leaked and had to be replaced. The plumber also recommended all the pipes in contact with the bricks be replaced because they were also corroded. Over the following decade the pipes had to be replaced twice and the second plumber suggested we check the soil pH which turned out to be between <3 ! We neutralised the soil and painted the walls around the HWS system with a weak caustic solution (sodium carbonate) and that seemed to solve the problem, well they never corroded after that.
The brickies assistant may have got overly enthusiastic with the brick cleaner and then never cleaned the residual down properly.
We can test this by leaving some of that demonised water exposed in clean container inside the shed and another outside the shed and after a week or so testing the pH (you can borrow my pH meter)
-
21st Jul 2019, 11:09 AM #28.
- Join Date
- Nov 2008
- Location
- Perth WA
- Age
- 71
- Posts
- 6,459
If only there was an assistant Bob!!! I never used anything other than my trowel to clean the bricks.
I discovered rust on the Acute's 1214 tool block yesterday. It, along with the remainder of the kit, had been stored in the cardboard Auspost box Gary posted the kit in and then more recently in a Systema plastic box. The corrosion took place inside the tin "shed" which is insulated and lined. So, I don't know.
IMG_20190721_080301312.jpg
-
21st Jul 2019, 12:57 PM #29Most Valued Member
- Join Date
- Nov 2007
- Location
- melbourne australia
- Posts
- 3,228
Should he have a priest on site when doing this Bob?
Bob,
Does your concrete floor have polythene underneath? If not, that would be where the moisture is coming from. Melbourne is considerably more moist than Perth and I get almost no corrosion on my tools and very little on my steel stock. You’ve got something going on there.Chris
-
21st Jul 2019, 01:49 PM #30Member: Blue and white apron brigade
- Join Date
- Feb 2006
- Location
- Perth
- Posts
- 7,189
I did a distance measurement on google earth and it's 300 odd meters difference, 700 for me and 400 for you. The other thing that might make a difference is the size of the land blocks. Where we are the small blocks means of the land is covered by roads and buildings whereas in your area with the bigger blocks there's more land to soak up and then evap water.
Similar Threads
-
Phosphating parts "experiment"
By Pete F in forum METALWORK GENERALReplies: 43Last Post: 17th Nov 2014, 10:46 PM -
A Saturday at the backyard foundry
By MuellerNick in forum THE FOUNDRYReplies: 64Last Post: 21st Aug 2012, 09:54 PM -
Professional black phosphating?
By neksmerj in forum METALWORK GENERALReplies: 4Last Post: 10th Aug 2012, 09:07 PM -
Backyard lineboring
By gallegos in forum METALWORK GENERALReplies: 9Last Post: 13th Dec 2010, 07:57 AM -
Backyard Foundry
By InkSpot in forum METALWORK GENERALReplies: 3Last Post: 10th Feb 2008, 07:40 PM