    Hi, I have been testing the thread cutting feature on my new HAFCO AL960-B Lathe.
    The threads work OK but the finish is terribly rough looking.
    I am running the speed at 170RPM -3/4" BSP 14TPI - Tool steel.
    I have watched Videos and amazed at how smooth the results others can get.
    I am using proper thread cutting tool (60deg)
    Any clues?
    Regards- Graham Hobbs

  2. #2
    Join Date
    Mar 2014
    Location
    South of Adelaide
    Posts
    1,227

    Default

    first off, wrong angle for bsp needs to be 55 not 60 degree. I'm assuming by proper threading tool you mean a carbide insert type tool? If so i have found that running dead slow 50ish or less revs can give a good finish, as the recommend cutting speeds aren't achievable on a manual lathe.

  3. #3
    Join Date
    Jul 2008
    Location
    near Warragul, Victoria
    Posts
    3,726

    Default more

    Sounds like the tool isn't sharp enough ? If using a HSS tool, a slight bit of side rake helps ( depending on the direction of the cut ) plus use a proper cutting fluid ie tap magic

  4. #4
    Join Date
    Sep 2006
    Location
    Australind , WA
    Age
    58
    Posts
    1,281

    Default

    I would have thought using cutting fluid would help?

  5. #5
    Join Date
    Jun 2007
    Location
    sydney ( st marys )
    Age
    64
    Posts
    4,890

    Default

    Are you plunge cutting or coming in at an angle using the compound?

  6. #6
    Join Date
    Jul 2021
    Location
    Sydney
    Age
    78
    Posts
    4

    Default Getting a smooth finish on threads

    Thanks everyone for your response.
    I am using a carbide insert tool.
    I will try the 55 degree tip as suggested and also try a better cutting fluid
    I will also drop the speed (if possible)
    Regards
    Graham

  7. #7
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    59
    Posts
    6,562

    Default

    Before doing any of that I would look at the material you are using. If it is just some garden variety 'mild steel' then it is quite likely that the threads will look torn. It's not always easy to find but if you want smooth looking threads then some 1214 (or 1214L) steel will give a nicer result.

    Michael

  8. #8
    Join Date
    Jul 2021
    Location
    Sydney
    Age
    78
    Posts
    4

    Default Getting a smooth finish on threads

    Thanks Michael.
    I am using Tool Steel.
    I have also tried a variety of materials with similar results.
    Cheers
    Graham

  9. #9
    Join Date
    Feb 2013
    Location
    Laidley, SE Qld
    Posts
    1,039

    Default

    My preferred method of single pointing threads is to cut 95% of thread depth on the lathe and then finish/polish with a die, assuming of course I have the correct die.

    An 85% deep cut allows you to cut most of a 55° thread with a 60° tool.

  10. #10
    Join Date
    Jan 2020
    Location
    Sydney
    Posts
    78

    Default

    I’ve done a fair amount of threading on my AL-960B using both inserts and HSS tools on different materials, and usually achieve reasonable results. One thing I always do if possible is use a live or dead centre to support the free end of the work piece, and of course make sure the gibs are tight and the tooling is exactly on centre height. Also having a variable speed drive helps a lot – lets me slow things right down when threading up to a shoulder then speed up when reversing back. I haven’t really noticed any difference in the finish depending on speed – more a function of the material and sharpness of the tooling.

Similar Threads

  1. surface finish
    By TED C in forum METALWORK GENERAL
    Replies: 9
    Last Post: 7th Aug 2015, 07:48 AM
  2. Help me finish my traytop
    By Bryan in forum TRAILERS & OTHER FABRICATED STUFF
    Replies: 47
    Last Post: 6th Aug 2015, 11:21 PM
  3. What finish is that?
    By neksmerj in forum METALWORK GENERAL
    Replies: 1
    Last Post: 24th May 2015, 09:18 PM
  4. Threads on finishing, finish, good finish
    By steamingbill in forum METALWORK GENERAL
    Replies: 17
    Last Post: 20th Jan 2014, 06:53 PM
  5. Rough finish
    By th62 in forum METALWORK GENERAL
    Replies: 16
    Last Post: 19th Jun 2013, 08:19 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •