Needs Pictures: 0
Results 1 to 14 of 14
-
25th Jan 2021, 10:47 AM #1Diamond Member
- Join Date
- Aug 2019
- Location
- Revesby - Sydney Australia
- Age
- 57
- Posts
- 1,195
What steel in car anti-roll bars?
Cleaning up a friend's garage, lots of bent, springy, steel:
IMG_1159.jpg
Variety of sizes (19/22/25mm).
Any idea what flavour?
I'm guessing not "spring steel", but if it is better than mild, I will cut out the straight sections and make a new drawbar
-
25th Jan 2021, 10:56 AM #2Most Valued Member
- Join Date
- Aug 2011
- Location
- Melbourne
- Posts
- 4,779
They are anti sway bars/ anti roll bars also known as stabiliser bars.
They are often removed from 4x4 vehicles when people heavily modify their suspension as they limit suspension travel.
I would think they would be made of spring steel since they perform a similar function.
Simon
Sent from my SM-G970F using TapatalkGirl, I don't wanna know about your mild-mannered alter ego or anything like that." I mean, you tell me you're, uh, super-mega-ultra-lightning babe? That's all right with me. I'm good. I'm good.
-
25th Jan 2021, 11:08 AM #3
I had a K-Mac on a a HK wagon.
For sure its 4140.
It made a hell of a difference. .
No idea how well it machines after it is heat treated, which the bars will be.
Grahame
-
25th Jan 2021, 11:19 AM #4Gear expert in training
- Join Date
- Aug 2008
- Location
- Melbourne
- Age
- 34
- Posts
- 1,080
This mob (and several other aftermarket manufacturers) say spring steel (5160) https://www.superproeurope.com/anti.roll.bars.cfm
Various other internet sources list 4340, 4130, 4140 and EN45 as well. Basically anything heat-treatable by the sound of it
-
25th Jan 2021, 06:41 PM #5Most Valued Member
- Join Date
- Nov 2017
- Location
- Geelong, Australia
- Age
- 57
- Posts
- 2,671
I made a chipping hammer out of an old HQ one back in the 80’s.
Hardened and tempered the hitting ends with the oxy torch and quenching in oil. It was hard as hell after quenching and definitely needed tempering back.
It’s held up really well over the years.
Steve
-
25th Jan 2021, 07:40 PM #6Diamond Member
- Join Date
- Aug 2019
- Location
- Revesby - Sydney Australia
- Age
- 57
- Posts
- 1,195
-
25th Jan 2021, 07:58 PM #7Gear expert in training
- Join Date
- Aug 2008
- Location
- Melbourne
- Age
- 34
- Posts
- 1,080
Which is apparently also 5160 by ASTM or 5155/5160 by AISI / SAE ... damn non-standard standards...
https://equivalentmaterials.com/materials/din-55cr3
-
25th Jan 2021, 10:59 PM #8Senior Member
- Join Date
- Aug 2011
- Location
- Perth, Western Australia
- Age
- 67
- Posts
- 362
From my old spec book AUST. STD AS1444-1979
XK5150S, XK5155S and XK5160S spring steel as BHP called them (= AISI-SAE 5150 5155 5160),
"The carbon chromium grades are used extensively for automotive suspension coil springs".
Over the page the same grades for non spring applications,
" Oil-hardening steels. Used for agricultural cultivators, coal cutter picks, die blocks, shear blades, punches and dies."
K1070S, K1082S (=SAE 1070 1082)
"The carbon grades uses include laminated rolling stock springs and automotive stabilizer bars".
I`d think it would come down to the application. Something like a 4x4 to me would need a spring steel because of the amount of twisting that`s going to be applied. Where as a sports car that has little twist something like a 4140 would do the job.
Tony
Just to clarify K1070S and K1082S are still spring steel they just don`t have the chrome content the others do.
-
10th Feb 2021, 08:17 PM #9Diamond Member
- Join Date
- Aug 2019
- Location
- Revesby - Sydney Australia
- Age
- 57
- Posts
- 1,195
Chopped off the curved bits:
IMG_1207.jpg IMG_1208.jpg
and tried turning.
IMG_1212.jpg
First, with my cheap carbide at 300RPM:
IMG_1213.jpg
then @500RPM:
IMG_1214.jpg
then 800RPM:
IMG_1215.jpg IMG_1216.jpg
(note the ring of worn-off steel - not a sharp cutter)
First one is my attempt. Just roughing cutters, but OK.
Second is my toolmaker friend, using iscar carbide+holder, coolant, and 900RPM:
IMG_1217.jpg IMG_1218.jpg
Definitely looks like it has a bit of Chromium in it!
-
10th Feb 2021, 08:26 PM #10Gear expert in training
- Join Date
- Aug 2008
- Location
- Melbourne
- Age
- 34
- Posts
- 1,080
That TNMG tool probably isn't doing you any favours.
I reckon CCMT is the way to go on small machines; they tend to be freer cutting which allows you to take the more aggressive depth needed to get a decent finish with less power.
-
10th Feb 2021, 09:04 PM #11Diamond Member
- Join Date
- Aug 2019
- Location
- Revesby - Sydney Australia
- Age
- 57
- Posts
- 1,195
True. It was just the first tool I grabbed. I also should have turned it to a fresh point (since there are 6 on each insert!).
Only CCMT I have is a boring bar which uses CCMT06es.
Next time, I might try a WNMG (although all my inserts are used WNMG06s).
Or maybe experiment with finishing off using round ones (RPMW 08).
-
10th Feb 2021, 09:09 PM #12Gear expert in training
- Join Date
- Aug 2008
- Location
- Melbourne
- Age
- 34
- Posts
- 1,080
Nothing wrong with using a boring bar for OD work if the shank is a decent size and it doesn't matter if the inserts are small, it's not like you'll be taking a cut big enough to max out an 06
-
10th Feb 2021, 10:07 PM #13Most Valued Member
- Join Date
- Nov 2017
- Location
- Geelong, Australia
- Age
- 57
- Posts
- 2,671
My first thought was that you're not taking a big enough DOC to get a decent finish.
My main turning tools are either WNMG08 or smaller CCMT - and for anything like that where its a bit unknown and likely to be a bit hard/tough I'd have a crack with the WNMG and a 0.5mm cut to see how it went first.
Steve
-
11th Feb 2021, 01:01 PM #14Most Valued Member
- Join Date
- Apr 2012
- Location
- Healesville
- Posts
- 2,129
Nigel this is pretty much the same material as what you have except that the axle might have been carburized so maybe a tougher skin.
The pic below is the axle that i recently turned to size, cant remember the feed rate but depth of cuts varried between .25 and .5mm, the gearbox was set to 275rpm and the vfd to 30hz, so about 150rpm.
I used coolant and the one corner of the insert (cnmg) to complete both ends of the job.
I dont use high rpm's very often as i am never in a hurry🤪
Similar Threads
-
Please help find near me - Stainless Steel Flat Bars 2mm x 12mm and 4mm x 12mm
By barrysumpter in forum METALWORK GENERALReplies: 10Last Post: 20th Jul 2020, 01:41 PM -
Anti Spam Filter
By wolfbunny in forum FORUMS INFO, HELP, DISCUSSION & FEEDBACKReplies: 1Last Post: 1st Nov 2014, 09:28 AM -
Anti-spatter spray
By Gavin Newman in forum WELDINGReplies: 8Last Post: 29th Apr 2012, 10:27 PM -
Help in finding a reliable source for square steel bars
By Cap'n Pharaoh in forum METALWORK GENERALReplies: 6Last Post: 1st Feb 2011, 11:03 PM -
Countersinking holes in steel bars
By JillB in forum METALWORK GENERALReplies: 8Last Post: 14th Oct 2009, 11:55 AM