    A family member has picked up about 30kg of brass (0.22 used rifle cartridges) from his gun club and wants to experiment with some small brass castings. He only has a small charcoal forge and couple of small (120 mL) graphite crucibles. He knows about needing to crush the cartridges before melting and yesterday we cut up a short length (70 mm) of 5mm wall x 40mm ID pipe (70mm) and made up a small press using a car jack. This doesn't seem to be working all that well - it seems like he'll need a heftier jack.

    A trial melting plan is to transfer some of the crushed cartridges to a 50 mm long piece of 25mm water pipe with a piece of steel welded to the bottom so it can stand up in the forge and just melt the brass inside the pipe. The question is - will the greater coefficient of thermal expansion of the brass (meaning the brass will shrink more when its cooled) allow for the solid bras slug to be removed say with a press?

    Apart from the obvious of careful inspection to make sure the cartridge is empty is there anything else he should be aware of. Is it worth the bother of cleaning the cartridges in something?

    His ultimate goal is to cast round nose brass heads for his long bow - these are around 11mm in diam x 19 mm long and have n short 8mm hole in the into which the arrow shaft is inserted - currently I turn these for him but I am over doing this.
    He'll almost certainly want to scale up from the charcoal forge to something a little larger whereby he can say cast 10 or 20 arrow heads at one time./

  2. #2
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    56
    Posts
    5,930

    Default

    Quote Originally Posted by BobL View Post
    A trial melting plan is to transfer some of the crushed cartridges to a 50 mm long piece of 25mm water pipe with a piece of steel welded to the bottom so it can stand up in the forge and just melt the brass inside the pipe. The question is - will the greater coefficient of thermal expansion of the brass (meaning the brass will shrink more when its cooled) allow for the solid bras slug to be removed say with a press?
    Probably, but you will have to see. It would help if the inside of the pipe was smooth (no fin) and tapered slightly outwards.

    Quote Originally Posted by BobL View Post
    Apart from the obvious of careful inspection to make sure the cartridge is empty is there anything else he should be aware of. Is it worth the bother of cleaning the cartridges in something?
    Any dirt will become slag on the top. Apart from the dangers of working with molten metal at around 900 degrees C, remember that the zinc will fume off from the brass, so the composition will change as well as the obvious health issues to be considered.

    Michael

  3. #3
    BobL is offline Member: Blue and white apron brigade
    Join Date
    Feb 2006
    Location
    Perth
    Posts
    6,450

    Default

    Thanks MG. Well he's had a go and reported back that he's made a "few scraggy looking molten blobs". I don't think he can control the temperature too well (or at all really) and he admits he needs a better heaT source.

  4. #4
    Join Date
    Dec 2014
    Location
    Tasmania
    Posts
    95

    Default

    Keep in mind that cartridge brass has approx 30% zinc content and will be giving off toxic fumes, more so than other brass like round stock or plumbing fittings.

    Have never melted spent cartridges but I have heard they dross badly, you lose a bit of brass. With tricky metals it helps to get a small molten pool going then feed into that, rather than load up the crucible from the start. Good luck!

  5. #5
    BobL is offline Member: Blue and white apron brigade
    Join Date
    Feb 2006
    Location
    Perth
    Posts
    6,450

    Default

    Thanks Ratters.

    I'm going to steer said relative away from experimenting with the rifle cartridges and instead use some old brass plumbing parts.

  6. #6
    Join Date
    Dec 2007
    Location
    Sydney
    Posts
    232

    Default

    When I was doing the Foundry course at Wollongong TAFE they wouldn’t put plumbing stuff in the pot. There were complete tap bodies in the 20 litre drum of scrap I had.
    They’d had explosions from water in taps.
    Be ok if you dismantle everything and preheat on the furnace lid.
    H.
    Jimcracks for the rich and/or wealthy. (aka GKB '88)

  7. #7
    Join Date
    Aug 2015
    Location
    QLD
    Posts
    735

    Default

    If yer chasing some cheap brass to melt down I’ve seen some cheap lots of large unused brass plumbing fittings and large door hinges, etc, going through the Pickles monthly military auctions.

    https://www.pickles.com.au/campaigns/ex-military/auctions/industrial/sale-type/Ex-Military/buy-method/Pickles%20Online/sort-by/custom-date-ascending/page/1


    Not items I’ve been bidding on so haven’t paid close attention though I think the items are navy related.

    Been a few lathes etc go through recently.




    .

  8. #8
    BobL is offline Member: Blue and white apron brigade
    Join Date
    Feb 2006
    Location
    Perth
    Posts
    6,450

    Default

    I gave the nephew some bits of plumbing and he managed to cast some small, sort of cylindrical shape,d blobs but now agrees that a small charcoal forge is not the way to do this. Im dreading him asking me to make something bigger.

Similar Threads

  1. casting a brass nut
    By kenny_10 in forum THE FOUNDRY
    Replies: 14
    Last Post: 27th Sep 2019, 01:45 PM
  2. Brass Casting, Poor Surface Finish
    By NedsHead in forum THE FOUNDRY
    Replies: 1
    Last Post: 30th Jul 2018, 12:40 PM
  3. Melting brass for lost wax casting
    By inlay chris in forum THE FOUNDRY
    Replies: 4
    Last Post: 17th Jun 2016, 09:06 PM
  4. Anyone have any experience casting brass?
    By Jim Ferrous in forum METALWORK GENERAL
    Replies: 7
    Last Post: 27th Sep 2013, 02:32 PM
  5. Casting a brass nut.
    By Skew ChiDAMN!! in forum METALWORK GENERAL
    Replies: 6
    Last Post: 21st Nov 2011, 01:04 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •