    Question First time casting aluminium, is my sand too wet?

    Hi all,

    I bought some greensand from Artisan Foundry but I can't seem to create a mould. I use talcum powder to help the two halves separate but it never comes apart cleanly like I've seen in demonstrations and any attempt to remove the part causes the sand to crumble.

    When I do the squeeze test it it tends to hold it's shape but it doesn't snap cleanly. Is my sand too wet? Or dry? Or some unholy mixture of the two?
    Any other advice you can give to a novice caster would be gratefully received as well.





  2. #2
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    59
    Posts
    6,561

    Default

    Welcome to the forum.

    One thing with green sand casting is that the sand has to be rammed in really hard. I mean really hard. It may be that it is crumbling because it has not been packed in enough.

    Michael

  3. #3
    Join Date
    Aug 2011
    Location
    Perth, Western Australia
    Age
    67
    Posts
    362

    Default

    I agree with Michael G, under ramming is a problem a lot of people have when using green sand.

    I have seen experienced moulders have trouble with greensand after coming across from CO2 or Furan sands.
    Practice more with different ramming pressures and don`t forget to add some gas vent holes.

    Tony

Similar Threads

  1. Sand casting
    By China in forum THE FOUNDRY
    Replies: 9
    Last Post: 11th Jan 2020, 12:37 AM
  2. First time aluminium casting
    By jhovel in forum THE FOUNDRY
    Replies: 10
    Last Post: 26th Apr 2016, 07:22 PM
  3. Regenerating oil bound casting sand
    By MuellerNick in forum THE FOUNDRY
    Replies: 11
    Last Post: 20th Jan 2013, 09:24 PM
  4. Vacuum assisted casting in core-sand moulds.
    By MuellerNick in forum THE FOUNDRY
    Replies: 22
    Last Post: 30th Oct 2012, 03:09 PM
  5. Casting Tools Part 4 - Sand Casting Tools
    By RayG in forum THE FOUNDRY
    Replies: 8
    Last Post: 9th Dec 2011, 12:03 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •