    Hi All,

    Just a quick overview of some of the tools used to prepare sand molds for casting, I'll leave patterns and cores for next time, these are just the tools used to do the preparation for the pour.

    First, I recommend petrobond for home hobby casting, it's an oil bonded sand, rather than "green sand" which is a water bonded sand. It's re-usable many times, and a bucket will last just about forever for home use. I got it from CMS, but I've since found they have changed names, I think they are now called "Arnott & Guy Foundry Supplies" 20-22 Marni St, DANDENONG SOUTH, VIC, 3175.



    The Queensland Address on the pail might still be the same..

    The consistency can change over time, and might require a touch extra oil, or sometimes I've added a squirt of iso-propanol, what you are looking for is when you grab a handfull, it packs cleanly and holds together nicely..



    Here is a quick overview of some of the tools used...



    Riddle (sieve) for removing clumps, scoops, rammers, scrapers, tubes for cutting sprues and risers, wire for making vent holes, trowell for cutting gates and parting lines, the sock is full of parting compound for dusting the pattern as well as the parting line in the cope and drag. The two screws are used to help remove split patterns from the sand. Also I'm told talcum powder works fine as a parting compound.



    The cope and drag, the drag is the bottom, and the cope is the top, together they are sometimes called a flask.. some flasks have snap connections on the corners. It's important that the cope and drag register accurately, that's what the triangle shaped bits on the side are for.



    Showing the two parts seperated..



    The best book for sand casting techniques, is CW Ammen, he covers patterns and casting strategies in some detail, the other is the Stephen Chastain book, which covers just about everything, but is a bit light on the casting strategy stuff..

    I'd recommend you get both.

    The next installment (part 5) will be making a pattern and preparing the cope and drag for casting.. that will demonstrate the use of the tools above...

    Regards
    Ray

  2. #2
    Join Date
    Jul 2006
    Location
    Athelstone, SA 5076
    Posts
    4,125

    Default

    Have'nt you got any thing to do Ray

    its great stuff

    I hope your saving all of this in word or something..It'd be great to see it as a pdf or similar after all the chapters are finished?

    PS dont forget the chapter on SAFETY
    Last edited by eskimo; 11th Nov 2011 at 09:34 AM. Reason: added safety bit

  3. #3
    Join Date
    May 2010
    Location
    Lower Lakes SA
    Age
    56
    Posts
    2,605

    Default

    Onya Ray. Don't think for a moment no replies means no interest. I've got my ears pinned back! And I'm sure many others do as well.

  4. #4
    Join Date
    Sep 2011
    Location
    Ballarat
    Age
    63
    Posts
    3,103

    Default

    What Bryan said Ray

    Phil

  5. #5
    Join Date
    Mar 2006
    Location
    Brisbane
    Age
    49
    Posts
    49

    Default

    I would just like to thank you for this Ray it may be something I never get to do but I find it very interesting indeed.
    I like to move it move it, I like to move it
    CNC Supplier List
    My Baby CNC

  6. #6
    Join Date
    Apr 2008
    Location
    Canberra
    Posts
    797

    Default

    Ray what do you do with the black, charred bits of petrobond after you have cast in it? I try to discard that bit, but by the looks of your photo theres a fair bit of black in that sand....do you just put the lot back in?

  7. #7
    Join Date
    Jun 2008
    Location
    Victoria, Australia
    Age
    72
    Posts
    5,080

    Default

    Quote Originally Posted by 19brendan81 View Post
    Ray what do you do with the black, charred bits of petrobond after you have cast in it? I try to discard that bit, but by the looks of your photo theres a fair bit of black in that sand....do you just put the lot back in?
    Hi Brendan,

    I used to do just that, scrape off the charred bits, and still do if it's a large lump that's easy to pick out, but over time more oil gets burnt off, and I add a bit of extra oil (doesn't take much) also a spritz with propanol seems to help keep the right consistency.

    So, by all means keep as much out as you can, but I don't think it's a deal breaker.

    Regard
    Ray

  8. #8
    Join Date
    Jul 2006
    Location
    Athelstone, SA 5076
    Posts
    4,125

    Default

    cant wait till this comes out in book form...need it for my library

  9. #9
    Join Date
    Apr 2008
    Location
    Canberra
    Posts
    797

    Default

    Thanks Ray

Similar Threads

  1. Casting Tools Part 2 - Burners
    By RayG in forum THE FOUNDRY
    Replies: 12
    Last Post: 12th Dec 2011, 10:07 AM
  2. Replies: 10
    Last Post: 7th Nov 2011, 01:27 PM
  3. Casting Tools Part 1
    By RayG in forum THE FOUNDRY
    Replies: 2
    Last Post: 3rd Nov 2011, 04:15 PM

Tags for this Thread

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •