I have to drill some 16mm holes through 2 x 6mm 316 stainless steel plates on a boat in situ. In fact the holes in question just need enlarging from 12mm to 16mm. I have a decent Black and Decker drill 500 watt/500 RPM and some stainless steel cutting paste. Would be interested if anyone has any tips/suggestions.
Thanks
Mike
-
7th Jun 2019, 08:30 AM #2Philomath in training
- Join Date
- Oct 2011
- Location
- Norwood-ish, Adelaide
- Age
- 59
- Posts
- 6,563
I think you would be better off getting a magnetic base drill (they can be hired). Clamp some steel plate onto the boat and use that. Handheld will work, but you do run the risk of the drill grabbing.
Good luck.
Michael
-
7th Jun 2019, 08:34 AM #3Most Valued Member
- Join Date
- Apr 2012
- Location
- Healesville
- Posts
- 2,129
Use a step drill.
-
7th Jun 2019, 10:21 AM #4Member: Blue and white apron brigade
- Join Date
- Feb 2006
- Location
- Perth
- Posts
- 7,189
Cobalt drill bit?
-
7th Jun 2019, 11:30 AM #5Senior Member
- Join Date
- Dec 2013
- Location
- Sydney
- Posts
- 201
This is a situation where I would use the folded piece of rag trick to stop the drill from chattering, keep it on centre and keep the hole round.
Graham.
-
7th Jun 2019, 02:15 PM #6Intermediate Member
- Join Date
- May 2019
- Location
- Tucson, Arizona, USA
- Posts
- 46
Hi Mike,
I like the idea of renting/borrowing a magnetic drill press (Mag Drill) mounted to a steel plate that is clamped to the stainless steel. You can use the existing hole size drill bit to center the drill, then switch out to the 16mm bit to enlarge the hole. I have several mag drills that I use for applications like yours. The mag drill in the first 2 photos has power feed, while the smaller one in the last photos has a drill chuck with manual down feed.
David
20190606_200224.jpg 20190606_200232.jpg 20190606_200239.jpg 20190606_200254.jpg
-
7th Jun 2019, 09:18 PM #7Senior Member
- Join Date
- Dec 2010
- Location
- Syd
- Posts
- 492
Enlarged some holes in 1/4 and 1/2" 316 about a year ago. not really a fun task by hand, just working the edges of the bit. Cobalt would usually do about 3~4 holes before trouble, masonry drill sharpened appropriately produced best results....avoid cooking the material at all costs, if you don't want to be drilling diamond!
-
7th Jun 2019, 09:58 PM #8Diamond Member
- Join Date
- Feb 2013
- Location
- Laidley, SE Qld
- Posts
- 1,039
Mark the 16mm circle, take out the 2mm margin with a carbide burr in a die grinder.
-
8th Jun 2019, 03:56 AM #9Novice
- Join Date
- Apr 2012
- Location
- Whitby, UK
- Posts
- 17
-
8th Jun 2019, 04:22 AM #10Novice
- Join Date
- Apr 2012
- Location
- Whitby, UK
- Posts
- 17
-
8th Jun 2019, 08:42 AM #11Most Valued Member
- Join Date
- Sep 2011
- Location
- Ballarat
- Age
- 65
- Posts
- 3,103
Hi Mike
High feed and low speed for stainless.
Phil
Similar Threads
-
Luck & Perspective.
By DSEL74 in forum GENERAL DISCUSSION / OFF TOPICReplies: 7Last Post: 16th Aug 2018, 11:26 AM -
WA day luck
By BobL in forum METALWORK GENERALReplies: 0Last Post: 1st Jun 2015, 08:38 PM -
Was this just good luck?
By BRADFORD in forum METALWORK GENERALReplies: 10Last Post: 8th Dec 2012, 12:52 PM -
I'm in love, wish me luck
By neksmerj in forum METALWORK GENERALReplies: 6Last Post: 2nd Dec 2010, 04:29 PM