    Default Parting off with small lathe

    I have a project which involves parting a piece of 60 mm stainless steel, my metal lathe is a small item AL 50g ( 9x20 )I did this several years ago and used a hacksaw NEVER AGAIN, I am going the parting off method this time. several people have said I would not be able to do this on such a small lathe.Well me being me I am going to do it anyway, I know to have it on on dead center, plus parallel to the work and to go slow anything else I should be aware of.

  2. #2
    Join Date
    Sep 2007
    Location
    Country West Oz
    Age
    77
    Posts
    169

    Default

    60mm stainless is a bit of an ask
    If your lathe can run in reverse, you might try putting the tool in upside down, I have found that works pretty well.
    Also your chance of success may depend on the type of parting tool. There are parting tools and there are parting tools.
    Regards
    Bradford

  3. #3
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    59
    Posts
    6,561

    Default

    Stainless commonly work hardens, so you need a decent rate of feed. On a small lathe that could be an ask. It also needs to be kept as cool as possible, so some form of coolant is a must.

    Michael

  4. #4
    Join Date
    Dec 2005
    Location
    South Australia
    Posts
    1,658

    Default

    Thanks for the replies, I will take note and let you know what transpires

  5. #5
    Join Date
    Sep 2012
    Location
    York, North Yorkshire UK
    Posts
    6,480

    Default

    Hi China,

    Good luck ! Even in mild steel a 30 mm stick out on a relatively thin blade is a big ask.
    Best Regards:
    Baron J.

  6. #6
    Join Date
    Jun 2012
    Location
    SA
    Posts
    1,649

    Default

    Good luck, cos you will need it.

    This is what will do it dead easy. A friction disc will cut it like a piece of cheese:

    https://www.youtube.com/watch?v=nYD5KbFA6EQ
    The worst that can happen is you will fail.
    But at least you tried.



  7. #7
    Join Date
    Jan 2004
    Location
    Mackay North Qld
    Posts
    6,446

    Default

    I don't know if your lathe has an automated, crossfeed.
    If it has not, you must hand feed at a constant rate.
    I part off up to 25 diameter 304 on a regular basis. For that, I use a 20mmx 3 HSS. The taper from top to bottom type.

    I use the sulphurised lube that is very thick. It helps to stop the lube being spun off.

    That sizing is the absolute limit on my 12x 36 as the toolpost flexes.

    I wish you good luck. Do wear your safety glasses, as I feel you may need them.

    Grahame

  8. #8
    Join Date
    Jun 2012
    Location
    SA
    Posts
    1,649

    Default

    Quote Originally Posted by Grahame Collins View Post
    I wish you good luck. Do wear your safety glasses, as I feel you may need them.

    Grahame
    Good point about the safety glasses Grahaeme.

    Parting off and using HSS drills on the lathe always makes me nervous. HSS can literally grenade under duress and I've had a large splinter of drill bit stick well into my forearm (through my heavy work shirt) on one occasion. Same thing with the drill press. When that stuff goes bang, it's not good.

    Play safe guys.
    The worst that can happen is you will fail.
    But at least you tried.



  9. #9
    BobL is offline Member: Blue and white apron brigade
    Join Date
    Feb 2006
    Location
    Perth
    Posts
    7,189

    Default

    The most significant thing that has improved my parting off ability has been to use "T" shaped cross section parting tools.

  10. #10
    Join Date
    Dec 2005
    Location
    South Australia
    Posts
    1,658

    Default

    Thanks for all the replies, I here you all, I chickened out and took it out the lathe and cut it on the cut off saw re chucked and cleaned it up

  11. #11
    Join Date
    Sep 2007
    Location
    Country West Oz
    Age
    77
    Posts
    169

    Default

    That's what I would have done.
    Quicker, easier and less stress.
    Regards
    Bradford

  12. #12
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    59
    Posts
    6,561

    Default

    Probably the best option.

    Michael

  13. #13
    Join Date
    Sep 2012
    Location
    York, North Yorkshire UK
    Posts
    6,480

    Default

    Hi China,

    Quote Originally Posted by China View Post
    Thanks for all the replies, I here you all, I chickened out and took it out the lathe and cut it on the cut off saw re chucked and cleaned it up
    That is exactly how I would have done it ! Much less stress.
    Best Regards:
    Baron J.

Similar Threads

  1. Replies: 19
    Last Post: 19th Mar 2014, 02:29 PM
  2. Paring with the lathe. (not parting)
    By Anorak Bob in forum METALWORK GENERAL
    Replies: 9
    Last Post: 11th Nov 2012, 08:30 PM
  3. On parting and rear mounted parting tools
    By Michael G in forum METALWORK GENERAL
    Replies: 8
    Last Post: 20th Oct 2012, 03:17 AM
  4. Recommend me a parting off tool for an AL-30 lathe.
    By faroogoo in forum METALWORK GENERAL
    Replies: 11
    Last Post: 9th Jul 2009, 08:55 PM
  5. Buying a lathe (Old massive Lathe, or New small C6 Lathe)
    By Ch4iS in forum METALWORK GENERAL
    Replies: 5
    Last Post: 25th Mar 2009, 12:19 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •