    The barrel key on my lathe tailstock was pretty worn and beat up allowing quite a bit of slop in the keyway, which does not really effect anything but, has always annoyed, me so I made a new one, or two, actually. This is a really simple part but requires quite a few different processes in it's manufacture.

    The first step was to turn and mill them slightly oversize to allow for final grinding to size after hardening. Material is EN36A,30mm Diameter.
    Old and New.jpg

    In the furnace at hardening temperature after previous pack carburising. I forgot to photograph the carburising process.
    Hardening temperature.jpg

    Quenching in Heat Transfer Oil.
    photo.JPG

    Hardness Testing - Result 60 Hrc.
    Hardness Test 1.jpgHardness Test 2.jpg

    Ready for grinding to final size.
    Parts Manual.jpg

    Grinding the O/D on a purpose built fixture after grinding the top and bottom surfaces.
    photo 1.JPG

    Grinding the actual key flanks to size.
    photo 2 (1).JPG

    The finished products and fixture.
    photo 3.JPG

  2. #2
    Join Date
    Oct 2004
    Location
    Southern Highlands NSW
    Posts
    1,898

    Default

    That's neat.
    Was the original key hardened?
    What grit is the grinding wheel you used? I'm curious as I want to buy the right one for my recently acquired surface grinder.

  3. #3
    Join Date
    Sep 2008
    Location
    Riddells Creek, Vic.
    Posts
    837

    Default

    Quote Originally Posted by nadroj View Post
    That's neat.
    Was the original key hardened?
    What grit is the grinding wheel you used? I'm curious as I want to buy the right one for my recently acquired surface grinder.
    Yes, the original was hardened and had been welded at some stage. The grinding wheel is a 60 grit aluminium oxide.

    Lex.

Similar Threads

  1. Replies: 0
    Last Post: 15th Mar 2015, 01:54 PM
  2. 9" tailstock barrel
    By Tonyau in forum THE HERCUS AREA
    Replies: 1
    Last Post: 9th Jan 2013, 12:13 PM
  3. Barrel Vice
    By barkersegg in forum GUNSMITHING
    Replies: 9
    Last Post: 31st Oct 2012, 04:52 PM
  4. Colchester
    By footz in forum METALWORK GENERAL
    Replies: 18
    Last Post: 1st Oct 2008, 10:42 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •