    Quote Originally Posted by NedsHead View Post
    Hi Joe

    I used 5lb potassium hydroxide, 2.5lb potassium nitrate, 1gal distiller water (although some water did evaporate while bluing), the time was approximately 25 minutes and the temp hovered around 140 C, it climbed a little as the water evaporated.

    I switched out the sodium hydroxide in the formula for potassium hydroxide because I have some on hand and I doubt it makes any difference, if I were to scale up the process I would use sodium hydroxide because it's considerably cheaper than potassium hydroxide

    Cheers

    At 140 degrees Celsius is the solution actively boiling ? ie bubbling and spitting and splashing droplets ?

    Bill

  2. #17
    Join Date
    Jan 2016
    Location
    Wodonga Vic
    Age
    33
    Posts
    366

    Default

    Hi Bill, at that temperature it's simmering, with all the salts dissolved in the solution it doesn't "bump" like boiling water does at 100C but it does spit small droplets around where it's being heated and release tiny caustic particles into the air that sting when they settle on skin, it's a well ventilated, covered skin and goggles affair

  3. #18
    Join Date
    Jun 2007
    Location
    Ipswich QLD
    Age
    63
    Posts
    1,621

  4. #19
    Join Date
    Sep 2011
    Location
    Emerald Central Qld
    Posts
    327

    Default

    This would be a good way to make shop made tooling last longer .And look better .

    Michael

  5. #20
    Join Date
    Aug 2010
    Location
    Near Bendigo, Victoria, AUS
    Age
    67
    Posts
    2,652

    Default

    I finally got some Potassium Nitrate yesterday. It was a special order and I had to leave my ful name, address, phone and license number to get it.
    Seems nobody bothers to stock it anymore because of these requirements.
    I won't have a chance to try and blue anything for a week or so, but will post the results here when I do.
    Cheers, Joe
    again completely retired - more time to contemplate projects and spend more shed time....

  6. #21
    Join Date
    Jan 2016
    Location
    Wodonga Vic
    Age
    33
    Posts
    366

    Default

    I look forward to seeing your results Joe, it's pretty pathetic what you had to go through just to get it, lets hope counter terrorism don't swoop your house over a bag of potassium nitrate lol

  7. #22
    Join Date
    Nov 2010
    Location
    Gippsland Victoria
    Posts
    620

    Default Potassium Nitrate

    Quote Originally Posted by jhovel View Post
    I finally got some Potassium Nitrate yesterday. It was a special order and I had to leave my ful name, address, phone and license number to get it.
    Seems nobody bothers to stock it anymore because of these requirements.
    I won't have a chance to try and blue anything for a week or so, but will post the results here when I do.

    I've tried too and anywhere I go they just say "No cannot get it any more - people were doing scary things with it"

    When I was a kid we could get Kwikcure from the local supermarket which was then used to cure meat and was pottassium nitrate

    This mob might be worth a try - am off on holidays and will try when I get back.

    kno3 potassium nitrate australia

    Bill

  8. #23
    Join Date
    Jan 2016
    Location
    Wodonga Vic
    Age
    33
    Posts
    366

    Default

    15 bucks a kilo, ouch... How much did you end up paying for a bag Joe?

  9. #24
    Join Date
    Aug 2010
    Location
    Near Bendigo, Victoria, AUS
    Age
    67
    Posts
    2,652

    Default

    I paid $71.40 for 25kg.
    Happy to share, if someone else wants a couple of kg ($3 a kg + postage).
    Cheers, Joe
    again completely retired - more time to contemplate projects and spend more shed time....

  10. #25
    Join Date
    Apr 2008
    Location
    NSW
    Posts
    543

    Default

    Yes they are talking about ammonium nitrate as a fertilizer however potassium nitrate is even more dangerous .
    You want Sodium Nitrate not Ammonium or Potassium nitrate .
    The volume of a pizza of thickness 'a' and radius 'z' is given by pi z z a.

  11. #26
    Join Date
    Jan 2016
    Location
    Wodonga Vic
    Age
    33
    Posts
    366

    Default

    How is a Potassium ion "even more dangerous" than a sodium ion? what is your measure of danger?

  12. #27
    Join Date
    Apr 2008
    Location
    NSW
    Posts
    543

    Default

    Potassium nitrate is a better oxidiser if it gets heated up by a fire . On it's own it's not so bad . It is used in explosives and some rocket fuels so it is very dangerous if it gets going in a fire .
    The volume of a pizza of thickness 'a' and radius 'z' is given by pi z z a.

  13. #28
    Join Date
    Aug 2010
    Location
    Near Bendigo, Victoria, AUS
    Age
    67
    Posts
    2,652

    Default

    All three are just fertilisers and meat tenderisers.
    Nothing dangerous about them at all - until you deliberately mix them with a fuel which they can oxydise. The mixtures and methods are not trivial and require research or reasonable chemistry knowledge. It is no more complex to make explosives or rocket fuel by many other means without resorting to fertiliser.....
    But these were easier to control (than, say, pool chlorine.....)
    Cheers, Joe
    again completely retired - more time to contemplate projects and spend more shed time....

  14. #29
    Join Date
    Nov 2008
    Location
    Perth WA
    Age
    66
    Posts
    6,112

    Default

    Hey Joe,

    I'll put my hand up for a couple of kilos if it's still available.

    Bob.

  15. #30
    Join Date
    Apr 2008
    Location
    NSW
    Posts
    543

    Default

    Anyway it's not Potassium nitrate you need in a bluing formula it's Sodium nitrate . To get the blotchy affect out you may need to degrease the metal before bluing it.
    The volume of a pizza of thickness 'a' and radius 'z' is given by pi z z a.

Page 2 of 3 FirstFirst 123 LastLast

Similar Threads

  1. My second attempt at steel bluing
    By BobL in forum METALWORK GENERAL
    Replies: 20
    Last Post: 4th Dec 2018, 02:25 PM
  2. More metal bluing
    By BobL in forum METALWORK GENERAL
    Replies: 59
    Last Post: 22nd Sep 2018, 11:04 PM
  3. Bluing a tapered shaft
    By jack620 in forum METALWORK GENERAL
    Replies: 20
    Last Post: 9th Apr 2013, 07:02 PM
  4. Bluing
    By bollie7 in forum METALWORK GENERAL
    Replies: 1
    Last Post: 28th Apr 2009, 10:37 PM
  5. Metal bluing solution
    By ohno in forum METALWORK GENERAL
    Replies: 28
    Last Post: 16th Dec 2006, 08:00 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •