Thanks: 0
Needs Pictures: 0
Picture(s) thanks: 0
Results 1 to 10 of 10
Thread: Cable Damascus
-
3rd Dec 2015, 09:15 AM #1
Cable Damascus
Yesterday I spent about five hours at the forge making this cable into a solid bar along with another piece about half the length.
It seems to have forge welded up nicely with no signs of inclusions or delimitations.
I need to prepare an enchant. There seems to be great controversy over the best acids, or combination and strength/dilution.
Hydrochloric, sulphuric, white vinegar, ferric, muratic.
So not sure what I will use yet.…..Live a Quiet Life & Work with your Hands
-
3rd Dec 2015, 09:32 AM #2
I forgot to mention that the bar reduced to bout a third the diameter of the original cable without much noticeable increase in length. Shows how much air is in between all the small strand twists and larger grouped twists making up the cable.
…..Live a Quiet Life & Work with your Hands
-
3rd Dec 2015, 01:49 PM #3
I drained some acid from an old battery and left it for an hour.
…..Live a Quiet Life & Work with your Hands
-
3rd Dec 2015, 02:11 PM #4
I am waiting to see how it looks when finished.
Dean
-
3rd Dec 2015, 08:13 PM #5Banned
- Join Date
- Aug 2015
- Location
- QLD
- Posts
- 735
The concept were new to me so I had a look-see at google pictures. Some amazing knife work made from old cables. I'm looking forward to seeing whats made here.
-
4th Dec 2015, 09:55 PM #6Golden Member
- Join Date
- Oct 2001
- Location
- ACT
- Posts
- 667
Looks nice. I have been wanting to give it a go myself. What process did you use etc. I have seen people combine a few length of cable - looks like yours was a decent diameter to begin with.
-
6th Dec 2015, 11:07 PM #7
I'm wondering what it will look like finished too….I'm also wondering what it will be as I haven't decided yet.
It's about 1" cable. The process is pretty simple.
Use tie wire to tie off each and to stop unravelling, cut length off.
Throw in coke forge heat to mid orange, coat heavily in borax and put back in forge, keep rotating the cable so it heats evenly and soaks through without burning the cable strands.
Pull out and lightly set the end, brush off, coat with borax put back in forge, fireweld ends and shape square may take a few heats, repeat other end.
heat whole length of cable to weld ing heat put one square end in vice and other in a shifter and twist the cable tighter. Brush..borax..heat. Start at one end and fireweld by hitting in a rotation following the cable Brush..borax..heat..reapt until solid. Forge to shape.…..Live a Quiet Life & Work with your Hands
-
17th Dec 2015, 07:35 PM #8Member
- Join Date
- Feb 2013
- Location
- Picton NSW
- Posts
- 82
That is coming along really nice!
Here is one of my cable damascus blades..
-
17th Dec 2015, 08:08 PM #9
Yeah nice job!
When are you doing a stall in melb next?…..Live a Quiet Life & Work with your Hands
-
17th Dec 2015, 08:11 PM #10Member
- Join Date
- Feb 2013
- Location
- Picton NSW
- Posts
- 82
Similar Threads
-
Does this cable contain Asbestos?
By variant22 in forum METALWORK GENERALReplies: 8Last Post: 24th May 2015, 11:04 AM -
VFD Remote Cable
By Oldneweng in forum METALWORK GENERALReplies: 18Last Post: 14th May 2014, 07:39 AM -
Damascus/ironwood knife
By ohno in forum KNIFE MAKINGReplies: 25Last Post: 18th Nov 2006, 11:17 AM -
damascus steel pendant
By ohno in forum METALWORK GENERALReplies: 4Last Post: 11th Nov 2006, 02:34 PM -
Hydrochloric acid for Damascus?
By ohno in forum METALWORK GENERALReplies: 10Last Post: 10th Oct 2006, 09:49 PM