    Seven or so years back I worked in a place that made stainless water heaters. Once the tanks were welded, they would be pickled with a Hydrofluoric/ Nitric acid mix. After hearing what it would do if splashed on skin I promised myself that I wouldn't go anywhere near something like that for the shed (there was the small children factor for a start).
    On the rare occasions I weld stainless (at home) I usually finish up with a wire brush or abrasive to take off the oxide. Does anyone know if anything been developed that can replace the HF/HNO3 mix that is relatively safe if spilt?

    Michael

  2. #2
    Join Date
    Dec 2010
    Location
    NINGI Qld Australia
    Age
    68
    Posts
    208

    Default

    I doubt if there is anything as effective but would like to hear if there is. I use it at home and hate the stuff but I am just careful, brush on very gentally, wear gloves and usually got my overalls and goggles, boots etc on anyway while welding. Yeah keep the billy lids and pets away for sure.

  3. #3
    Join Date
    Jan 2011
    Location
    Far West Wimmera
    Age
    63
    Posts
    4,049

    Default

    The latest method as far as I am aware involves using an electronic machine with a wand of some kind and a liquid. I have seen it used at work by maintenance and contractors. It is safer than the old mix which is the stuff of nightmares but I cannot be more specific. I have my doubts whether it is viable for hobby use but that is not based on actual knowledge so don't think it is. If anyone is really interested I could ask some questions.

    Dean

  4. #4
    Join Date
    Dec 2005
    Location
    Canberra
    Posts
    490

    Default

    Here's the wand kind of pickle...

    It's a form of electrolytic cleaning - phosphoric and citric acid + current.

    [ame=http://www.youtube.com/watch?v=NoKa4TBxmRE]Pickling Stainless Steel: Stainless steel fabricators in a pickle no longer - YouTube[/ame]

  5. #5
    Join Date
    May 2008
    Location
    Sydney
    Posts
    79

    Default

    Aussie developed and Aussie made.

    Metal Science Technologies | mepBLITz

    Cheers
    Pete

  6. #6
    Join Date
    Jan 2011
    Location
    Far West Wimmera
    Age
    63
    Posts
    4,049

    Default

    Well there you go. Next question is how much?

    Dean

  7. #7
    Join Date
    Aug 2010
    Location
    Glenbrook NSW Australia
    Posts
    125

    Default

    Quote Originally Posted by Oldneweng View Post
    Well there you go. Next question is how much?

    Dean
    Found some prices

    FOR SALE:VIC Surfox Weld Cleaner & Etching Attachment [Archive] - Woodwork Forums
    http://phillytool.com/Merchant2/merc..._Code=AWALTERN

    mmmm

    Russell
    vapourforge.com

  8. #8
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    59
    Posts
    6,559

    Default

    Interesting stuff guys - I picked up a price on the 'net of $8 to $9k for the big brother unit to the one shown in the video. I have an email in to see what the smaller version (the one shown in the video) will set a buyer back.

    The added bit - Still not cheap. Even the baby Surfox unit is still $1800 ish. Looking at these though I'm now wondering how sophisticated they are. The lunchbox size inverters are getting common and cheaper too (a several hundred dollars). The rest of the set up doesn't look very complicated. While not as good as a purpose designed unit, would that work for an occasional user? Thoughts?

    Michael
    Last edited by Michael G; 21st Jul 2012 at 08:38 AM. Reason: looked at Russell's links

  9. #9
    Join Date
    Jan 2011
    Location
    Far West Wimmera
    Age
    63
    Posts
    4,049

    Default

    I did a bit of googling and came up with
    TIG Welder for Stainless Weld Discoloration Removal

    I happen to have both phosphoric and citric acid already. May be I will try with my little battery charger. One day. Am very interested in anybody else posting their results. I am trying to clean up my shed not make more mess LOL.

    Dean

  10. #10
    Join Date
    Aug 2004
    Location
    Lost in Space
    Age
    53
    Posts
    331

    Default

    I must be missing something here why not simply polish it there a many different methods that can be used to polish stainless upto a mirror finish...............and best of all no fiendish chemicals!!!!

    Regards Lou
    Just Do The Best You Can With What You HAve At The Time

  11. #11
    Join Date
    Jan 2011
    Location
    Far West Wimmera
    Age
    63
    Posts
    4,049

    Default

    Quote Originally Posted by NewLou View Post
    I must be missing something here why not simply polish it there a many different methods that can be used to polish stainless upto a mirror finish...............and best of all no fiendish chemicals!!!!

    Regards Lou
    It is not enough to polish the surface. It has to be treated to protect it and stop rust forming. This is the reason for the chemicals etc. Others may be able to provide more detail.

    Dean

  12. #12
    welding is offline Engineers are qualified to make claims
    Join Date
    Dec 2010
    Location
    Victoria
    Posts
    81

    Default

    I believe that contaminants stop chromium oxide molecules forming as the protective barrier. SS needs oxygen to get to the surface in order to form the chromium oxide. Contaminated surfaces after welding prevent oxygen getting to the chromium which can then allow it to rust. You can often see on dirty stainless steel there is a brown rust formation known as tea staining, this is because oxygen is not able to get to the chromium in those areas to form the protective barrier.


    Regards
    John

  13. #13
    Join Date
    Sep 2010
    Location
    Lebrina
    Posts
    1,914

    Default

    I am glad to see the healthy respect that is being shown for pickling paste - it truly is fiendish stuff.
    The electrolytic methods work really well, but at a high set up cost.
    Tecnically, to gain the utmost corrosion resistance you are supposed to pickle and neutralise, which is a two step process. Most skip the neutralising step in my experience.
    To be honest, unless the environment is really nasty, I have never seen too much go awry after a good wire brush (stainlless brush of course) or a rub with a scotchbrite pad. As far a polishing stainless goes, it's a mongrel job! Plus once polished you must maintain it or it gets daggy looking and show marks etc. A brushed finish is probably a little more user friendly and much faster to achieve while hiding effectively any small blemishes etc. A full on polish will show every surface blemish and ripple.
    If pickling is a must, then use good chemical gloves and a full face mask - safety glasses just don't cut it, (you can also get a neutralising solution for use in a first aid scenario but it is very expensive and has a limited life I believe) and make sure that you use plenty of water to dilute any residue, (hot water seems to work best when washing the solution off by the way).
    The need to pickle can be minimised by correct amperage settings - don't get the weld too hot or you get really thick black oxides, the rainbow hues are what you want to see and consider purge welding components to provide a gas cover on the root side of the weld.

  14. #14
    Join Date
    Oct 2011
    Location
    Norwood-ish, Adelaide
    Age
    59
    Posts
    6,559

    Default

    Got an email back on the Aussie made electrolysis units. The TIG champ retails for around $3k and the megaBlitz is around $5k.

    Not cheap. Perhaps it's the wire brush after all.

    Michael

  15. #15
    Join Date
    Mar 2010
    Location
    Nth Qld
    Posts
    687

    Default

    I looked up stainless passivation earlier this year and found an article that said to use 30% nitric acid in water. It made the steel shot blasted 316 that had gone tea brown after a day in the rain, go silver white in appearance and it's been fine for the last 5 months or so. I did several coats and rinsed off in between with the hose so the it didn't dry out with acid on it. Nitric is an oxidising acid apparently.